Reflow soldering will have various failures during work. Among them, the reflow soldering chip wicking phenomenon is one of the problems. Below, Guang Shengde will briefly analyze the reflow soldering wicking problem.


20190621043936600.jpg

Reflow wicking

1.The positive temperature of reflow soldering is higher than the back temperature.

In the reflow soldering process, the reflow temperature should be set according to the material, size, component specifications and component density of the PCB. Of course, it also depends on whether it is a double-sided soldering process. If the PCB is thinner and the size is smaller, When doing the double-sided soldering process, a 128PIN or larger QFP must be mounted. This issue must be taken into account when setting the temperature.


Because in the double-sided soldering process, it is necessary to consider that the back component will have high parts or even drop parts due to the secondary reflow. Therefore, the back temperature setting should be slightly lower than the positive temperature. But if the setting is improper, the back temperature is lower than the positive temperature. If the temperature is too much, the result is that the PCB heat is lower, and the component heat is higher. Due to the flow of the solder after melting, the solder will naturally not adhere to the PAD, but to the pins of the QFP with high temperature. When it climbs up, the phenomenon that occurs is that the PAD has less tin and the QFP's pins are bridged and connected to the tin.


2.PAD oxidation.

If the OSP material PCB is not put into production on the BOT surface in time (24 hours) after the TOP surface is completed, then the PAD will be oxidized, and the PAD's ability to eat tin will be severely reduced during soldering. Of course, the solder will climb to the pins of the component. As a result, the pins of the PAD less tin component are connected to the tin.


The above reflow soldering chip wicking countermeasures:


1.When setting the reflow soldering temperature, the difference between the positive temperature and the back temperature is controlled at 15, and the measured temperature difference is controlled at 5 degrees.


2. Use two production lines, and put the BOT surface into production immediately after the TOP surface is completed. If two lines cannot be opened, the produced PCB must be moisture-proof.

国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 日本欧美在线视频观看-国产一区二区三区无码下载快播| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 天天日天天干天天综合-99久久综合狠狠综合久久| 日本少妇激情一区二区-亚洲自偷自拍熟女另类蜜臀| 蜜臀一区二区三区精品在线-99久久久精品免费看国产| 亚洲av乱码一区二区-九九免费在线观看视频| 深夜三级福利在线播放-日韩精品一区二区在线天天狠天| 亚洲中文一二三av网-亚洲天堂成人免费在线| 国产剧情av中文字幕-五月婷婷在线手机视频| 中文字幕亚洲中文字幕-丰满老妇伦子交尾在线播放| 中文字幕偷拍亚洲九色-亚洲视频不卡一区二区天堂| 国产精品熟女视频一区二区-国产日韩精品欧美一区喷水| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 国产在线一区二区三区欧美-久久偷拍精品视频久久| 久久网站中文字幕精品-三级精品久久中文字幕| 天天干天天干2018-91人妻人人澡人爽精品| 久久久国产精品电影片-精品孕妇人妻一区二区三区| 成人免费资源在线观看-欧美国产日韩高清在线综合| 99久热精品免费观看四虎-亚洲天堂精品视频在线| 天天干天天干2018-91人妻人人澡人爽精品| 色综合色综合久久综合频道-埃及艳后黄版在线观看| 日韩亚洲一区二区三区av-欧美综合在线观看一区二区三区| 黑丝av少妇精品久久久久久久-中文字幕久久久人妻无码| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 7m视频7m精品视频网站-亚洲综合香蕉视频在线| 免费av一区在线观看-国产精品视频高潮流白浆视频免费| 日韩中文字幕v亚洲中文字幕-日韩亚洲av免费在线观看| 欧美精品午夜一二三区-a屁视频一区二区三区四区| 99在线免费观看视频-丰满人妻一区二区三区视频53| 午夜福利1区2区3区-午夜洗澡免费视频网站| 日韩精品一区二区三区粉嫩av-欧美亚洲国产中文字幕| 美女把腿张开给帅哥桶-无码无套少妇18p在线直播| 黄片一区二区三区在线看-偷拍一区二区在线观看| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 国产精品一区二区欧美视频-国产一区二区三区天码| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 99在线观看精品视频免费-国产极品一区二区三区四区| 乱入一二三免费在线观看-久久精品亚洲精品国产色婷婷| 久久精品亚洲无中文东京热-日本妹子内谢视频一区| 国产免费一区二区三区不-日本少妇免费一区二区三区|